Ceramics-Silikáty 35, (4) 335 - 340 (1991) |
|
PREPARATION OF ALUMINA MEMBRANES FOR MICROFILTRATION |
Fellner Pavel 1, Haviar Miroslav 2, Koman Marián 1,
Chovancová Marta 1 |
1 Department of Inorganic Technology, Slovak Technical University, Radlinského 9, 812 37 Bratislava, Czechoslovakia
2 Institute of Inorganic Chemistry, Slovak Academy of Sciences, Dúbravská cesta, 842 36 Bratislava, Czechoslovakia
|
Porous α-Al₂O₃ ceramics for microfiltration membranes can he obtained by calcination of Al(OH)₃ in the temperature interval 1150 – 1400 °C followed by milling and sintering. Calcination at 1150 °C provides θ-Al₂O₃ whose sintering leads to approx. 8 % higher porosities comparing to α-Al₂O₃. Milling of calcined powder has significant influence on decreasing of the mean pore size which is accompanied by the 20-25 % decreasing of porosity. |
PDF (2.8 MB) |
|